Process Key Points for PPS High-temperature Material Injection Molding

2026-11-23 11:36:03 Injection Molding

PPS is a crystalline high-temperature engineering plastic. Glass fiber reinforced grades are widely used in automotive electronics, connectors and high-temperature resistant structural parts. It has a narrow molding window and is highly sensitive to moisture, temperature and shear. Slight parameter fluctuation may cause silver streaks, black spots, floating fiber, dimensional drift and weak weld lines. The core of molding control is sufficient drying, stable mold temperature, limited melt residence time, as well as matched wear-resistant and corrosion-resistant molds and injection machines.

1. Raw Material Drying Control

PPS has low water absorption, but trace moisture will cause material degradation under high melt temperature, resulting in bubbles, silver marks and surface defects, so drying cannot be skipped. Dehumidifying dryers are recommended, with drying temperature set at 140℃ to 150℃ for 4 to 6 hours, and dew point kept below -30℃. Ordinary hot air drying easily leads to re-absorption of moisture. The regrind material addition ratio should be controlled within 20%. Regrind needs to be mixed with virgin material and dried together. Repeated recycling will greatly reduce mechanical performance, so it is not suitable for high-strength and high-reliability components. The feeding throat is equipped with water cooling to prevent premature melting and bridging, ensuring stable feeding.

injection mould

2. Barrel and Melt Temperature Control

Unfilled PPS barrel temperature ranges from 300℃ to 325℃. Glass fiber reinforced grades are adjusted to 310℃ to 340℃, with gradient heating from rear zone to nozzle. The nozzle temperature is slightly higher than the front zone to avoid cold material blockage. Melt temperature should not stay above 340℃ for a long time. Once it exceeds 360℃, crosslinking and carbonization will occur, causing black spots and brittle products, and accelerating corrosion of screw and check ring. Melt residence time in the barrel must be strictly controlled. The shot size should reach 30% to 50% of machine capacity. If the shutdown lasts more than 15 minutes, lower the barrel temperature or empty the barrel. For long shutdown, use PP or PE to clean the barrel to prevent residual PPS carbonization.

3. Mold Temperature Control

Mold temperature is the most critical parameter for PPS molding, which directly determines crystallinity, dimensional stability, chemical resistance and mechanical performance. For glass fiber reinforced PPS, the recommended mold temperature is 130℃ to 150℃, and oil-type mold temperature controllers are preferred. Ordinary water chillers cannot stabilize this temperature range. Low mold temperature leads to incomplete crystallization, large internal residual stress, continuous post-shrinkage after molding, deteriorated solvent resistance and heat resistance. The mold temperature must be uniform, and cooling channels are arranged close to the cavity to reduce local temperature difference. For thick-wall products, properly raise the upper limit of mold temperature to synchronize crystallization and reduce warpage risk.

4. Injection, Packing and Cooling Parameters

PPS melt has low viscosity and suits medium-high filling speed of 40 to 80 mm/s. Multi-stage speed setting is adopted, and slow down near the gate to reduce shear heat, jetting marks and floating fiber. Injection pressure is set from 80 to 150 MPa according to product structure. Higher glass fiber content requires higher injection pressure. Packing pressure is 50% to 70% of injection pressure, and position switch packing is better than time switch for stable feeding. Packing time increases with wall thickness. Back pressure is 3.5 to 7 MPa and screw speed is 80 to 120 rpm. Excessive back pressure and rotating speed bring extra shear heat, worsening floating fiber and degradation. Cooling time must match crystallization progress. After ejection, products are placed on flat jigs for natural cooling and shaping to avoid warpage.

5. Mold Structure and Venting Requirements

Glass fiber reinforced PPS causes heavy mold wear, so S136 or STAVAX corrosion-resistant and wear-resistant steel is preferred for cavity and core. Nitriding treatment can be adopted when necessary. Venting depth is controlled at 0.02 to 0.03 mm, set at weld convergence positions and filling end areas. PPS will release sulfur-containing gas under high temperature, and poor venting easily causes burning and brittle weld lines. Side gates and fan gates are recommended to reduce shear. Thin-wall precision parts can adopt hot runners, and the hot runner temperature keeps consistent with nozzle temperature.

injection mould

6. Common Defects and Daily Production Control

Floating fiber is mainly caused by excessive shear and low mold temperature, which can be improved by raising mold temperature and reducing screw speed and back pressure. Weak weld lines need optimized venting, higher mold temperature and overflow wells. Black carbonization spots are mainly caused by overhigh temperature and long residence time. Dimensional fluctuation focuses on mold temperature stability, drying status and packing switch position. During mass production, first-piece, patrol and final-piece inspection is implemented. Screw and check ring wear should be checked regularly to prevent unstable metering.

7. Shutdown and Material Change Specification

For short shutdown, reduce barrel temperature by 20 to 30℃ and perform empty shot periodically to avoid melt carbonization. Empty the barrel completely for long shutdown and use purging compound to clean residual PPS. When switching to other materials, fully clean the barrel, and shoot empty shots before formal production to confirm no black spots or impurities.

injection mould